其它 其它 注塑 | |
特性:中等粘度,热稳定性,耐气候性,延性。 |
性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | ||
吸水率 | 23℃,24小时 | ASTM D-570 | 无水|1.8 | % | |
吸水率 | 23℃,24小时 | ASTM D-570 | 3.5%水|- | % | |
泰伯磨耗量 | 1000g,CS-17 | ASTM D-1044 | 无水|3-4 | mg/1000次 | |
泰伯磨耗量 | 1000g,CS-17 | ASTM D-1044 | 3.5%水|- | mg/1000次 | |
比重 | ASTM D-792 | 无水|1.12-1.14 | |||
比重 | ASTM D-792 | 3.5%水|- | |||
抗剪强度 | 23℃ | ASTM D-792 | 无水|720 | Kg/cm2 | |
抗剪强度 | 23℃ | ASTM D-792 | 3.5%水|650 | Kg/cm2 | |
抗拉屈服强度 | 80℃ | ASTM D-638 | 无水|270 | Kg/cm2 | |
抗拉屈服强度 | 80℃ | ASTM D-638 | 3.5%水|200 | Kg/cm2 | |
挠曲模量 | 23℃ | ASTM D-790 | 无水|25000 | Kg/cm2 | |
挠曲模量 | 23℃ | ASTM D-790 | 3.5%水|8000 | Kg/cm2 | |
IZOD冲击强度 | 23℃,无缺口1/8 | ASTM D-256 | 无水|6.5 | kg.cm/cm | |
IZOD冲击强度 | 23℃,无缺口1/8 | ASTM D-256 | 3.5%水|<50 | kg.cm/cm | |
挠曲模量 | 80℃ | ASTM D-790 | 无水|7000 | Kg/cm2 | |
挠曲模量 | 80℃ | ASTM D-790 | 3.5%水|3000 | Kg/cm2 | |
断裂伸长率 | 23℃ | ASTM D-638 | 无水|<200 | % | |
断裂伸长率 | 23℃ | ASTM D-638 | 3.5%水|<200 | % | |
挠曲模量 | -40℃ | ASTM D-790 | 无水|39000 | Kg/cm2 | |
挠曲模量 | -40℃ | ASTM D-790 | 3.5%水|37000 | Kg/cm2 | |
IZOD冲击强度 | 23℃,无缺口1/8 | 无水|无裂断 | kgcm/cm2 | ||
IZOD冲击强度 | 23℃,无缺口1/8 | 3.5%水|- | kgcm/cm2 | ||
洛氏硬度 | 80℃ | ASTM D-785 | 无水|80 | R-标度 | |
洛氏硬度 | 80℃ | ASTM D-785 | 3.5%水|- | R-标度 | |
压缩强度 | 23℃ | ASTM D-695 | 无水|820 | Kg/cm2 | |
压缩强度 | 23℃ | ASTM D-695 | 3.5%水|650 | Kg/cm2 | |
抗拉屈服强度 | 23℃ | ASTM D-638 | 无水|760 | Kg/cm2 | |
抗拉屈服强度 | 23℃ | ASTM D-638 | 3.5%水|350 | Kg/cm2 | |
挠曲强度 | -40℃ | ASTM D-790 | 无水|1400 | Kg/cm2 | |
挠曲强度 | -40℃ | ASTM D-790 | 3.5%水|1300 | Kg/cm2 | |
抗拉屈服强度 | -40℃ | ASTM D-638 | 无水|1130 | Kg/cm2 | |
抗拉屈服强度 | -40℃ | ASTM D-638 | 3.5%水|1000 | Kg/cm2 | |
IZOD冲击强度 | -40℃,无缺口1/2 | ASTM D-256 | 无水|4.5 | kg.cm/cm | |
IZOD冲击强度 | -40℃,无缺口1/2 | ASTM D-256 | 3.5%水|- | kg.cm/cm | |
挠曲强度 | 80℃ | ASTM D-790 | 无水|430 | Kg/cm2 | |
挠曲强度 | 80℃ | ASTM D-790 | 3.5%水|250 | Kg/cm2 | |
洛氏硬度 | 23℃ | ASTM D-785 | 无水|119 | R-标度 | |
洛氏硬度 | 23℃ | ASTM D-785 | 3.5%水|88 | R-标度 | |
挠曲强度 | 23℃ | ASTM D-790 | 无水|1000 | Kg/cm2 | |
挠曲强度 | 23℃ | ASTM D-790 | 3.5%水|400 | Kg/cm2 | |
抗拉断裂强度 | 23℃ | ASTM D-638 | 无水|800 | Kg/cm2 | |
抗拉断裂强度 | 23℃ | ASTM D-638 | 3.5%水|520 | Kg/cm2 | |
体积电阻率 | ASTM D-257 | 无水|1013-1014 | Ω.cm | ||
体积电阻率 | ASTM D-257 | 3.5%水|1011-1012 | Ω.cm | ||
UL-94抗燃级 | UL 94 | 无水|HB(1/16) | |||
UL-94抗燃级 | UL 94 | 3.5%水|- | |||
热挠曲温度 | 4.6kg/cm2 | ASTM D-648 | 无水|182 | ℃ | |
热挠曲温度 | 4.6kg/cm2 | ASTM D-648 | 3.5%水|- | ℃ | |
比热 | 无水|0.46 | Cal/g℃ | |||
比热 | 3.5%水|- | Cal/g℃ | |||
线性热膨胀系数 | ASTM D-696 | 无水|8 | ×10-5cm/cm/℃ | ||
线性热膨胀系数 | ASTM D-696 | 3.5%水|- | ×10-5cm/cm/℃ | ||
导热系数 | 无水|0.18 | Kcal/mhr℃ | |||
导热系数 | 3.5%水|- | Kcal/mhr℃ | |||
熔点 | 差示扫描测热计DSC | 无水|225 | ℃ | ||
熔点 | 差示扫描测热计DSC | 3.5%水|- | ℃ | ||
关于日本东丽 CM1026价格 | |||||
1.有关“PA6 日本东丽 CM1026”物性表及PA6塑料颗粒价格以出厂实时数据为准. 2.更多塑料原料的需求请与我们联系,电话同微信:186-2131-7168 |
本文链接:http://www.28at.com/showinfo-41-15249-0.htmlPA6 日本东丽 CM1026
声明:本网页内容旨在传播知识,不代表本站观点,若有侵权等问题请及时与本网联系,我们将在第一时间删除处理。
上一篇:PA6 日本东丽 UTN121
下一篇:PA6 日本东丽 CM1021